    Default PowerPro 205 - first BIG welds - porosity issues resolved

    Well, the issues I had with Porosity are now gone. Seems like there were a host of little thing that were working against me. Any one of them could have caused the problem. Hoses, insificient cleaning - inside and out, bad gas and technique - probably in combination with each other.

    Well, tonight, with hoses replaced, new gas, flow set to 7.5L/min and VERY CLEAN material, I sharpened-up a 1/16" electrode and tried it again.

    I built a simple joint of 1/4" mild steel and vola! This is a combination of 3 welds. No porosity at all.

    I'm sure the pros will point out issues with this weld but, for a 25-year broadcast engineer and 2 month welder, I didn't think this was half bad.

    Critiques Welcome!
    Click image for larger version. 

Name:	IMG_3679.jpg 
Views:	533 
Size:	127.0 KB 
ID:	6295
    Last edited by inthefrey; 04-20-2012 at 04:53 AM.

  2. #2

    Default

    Looks much better!

    You will probably fair a bit better on teh thick stuff if you use a lager diameter tungsten (3/32 or so).
    Everlast 200DX
    Everlast PT185
    Shoptask 3-in-1 (not currently in my garage, but I own it...)

    Any day on a motorcycle like this that ends just needing parts and labor is a good day.
    4.82, 158.67mph 1/8th mile 7.350, 200.35mph 1/4 mile

  3. #3

    Default

    Quote Originally Posted by sportbike View Post
    Looks much better!

    You will probably fair a bit better on teh thick stuff if you use a lager diameter tungsten (3/32 or so).
    I agree,,,the weld looks cold,,,

    inthefrey,,,here is a site with a Tech manual that will be of great help in choosing electrodes, cupsizes, litre flows and Amp settings
    The information most helpful to you are at the bottoms of page 3,,4,, and 6 of the manual,,,,great reading for a new tig guy...


    http://www.ckworldwide.com/technical.htm

    if you study the charts you can see there is a relationship to cupsize and litreflow,,,they very near the same,,etc,,,,also you can see that electrode size and cup size have their limits and ranges....just plain old good reading to understand how to set up your machine...
    Some of those lies people tell about me, are true

  4. #4
    Join Date
    Mar 2012
    Location
    Western Pennsylvania
    Posts
    63

    Default

    Quote Originally Posted by geezer View Post
    I agree,,,the weld looks cold,,,

    inthefrey,,,here is a site with a Tech manual that will be of great help in choosing electrodes, cupsizes, litre flows and Amp settings
    The information most helpful to you are at the bottoms of page 3,,4,, and 6 of the manual,,,,great reading for a new tig guy...


    http://www.ckworldwide.com/technical.htm

    if you study the charts you can see there is a relationship to cupsize and litreflow,,,they very near the same,,etc,,,,also you can see that electrode size and cup size have their limits and ranges....just plain old good reading to understand how to set up your machine...
    Many thanks! You know, there are probably a dozen possible combinations that will work.

    I wish I had taken a picture of the root pass. It was awesome! As I said, this was the 3rd weld on this joint and, you're right, I probably didn't have enough heat on it. As far as the various welding sites are concerned, you can never really learn all there is to know by watching all the videos and reading all the text - you have to DO it and develop your own "style" and become ONE with your machine.

    The weldingtipsandtricks site is about the most comprehensive. However, you're watching a guy (jody) with 30+ years of experience trying to teach adult noobs like me how to weld. ( I can see me now in a class with a bunch of 19-year-olds )

    Anyway, I'm having more fun doing and learning this than a human should be allowed.

    Thanks all for all the great pointers! Now, back to the bench! I'll post more stuff soon!~

    inthefrey

  5. #5

    Default

    Quote Originally Posted by inthefrey View Post
    Many thanks! You know, there are probably a dozen possible combinations that will work.

    I wish I had taken a picture of the root pass. It was awesome! As I said, this was the 3rd weld on this joint and, you're right, I probably didn't have enough heat on it. As far as the various welding sites are concerned, you can never really learn all there is to know by watching all the videos and reading all the text - you have to DO it and develop your own "style" and become ONE with your machine.

    The weldingtipsandtricks site is about the most comprehensive. However, you're watching a guy (jody) with 30+ years of experience trying to teach adult noobs like me how to weld. ( I can see me now in a class with a bunch of 19-year-olds )

    Anyway, I'm having more fun doing and learning this than a human should be allowed.

    Thanks all for all the great pointers! Now, back to the bench! I'll post more stuff soon!~

    inthefrey
    Glad to help,,,and you are right it's practice, practice ,,,practice,,,,nobody became a great lover by just reading playboy,,,,you actually have to get out there and do it...today I welded like a 19 year old,,,,a totally braindead day,,,it was like who put a stinger in the hand of this retard,,,,oh well I probably needed to practice my grinding anyhow..LOL ,,,somedays a guy should stay in bed....
    Some of those lies people tell about me, are true

Similar Threads

  1. New 185dv owner with a porosity issue
    By Deep Six in forum TIG Welding (GTAW/GTAW-P)
    Replies: 40
    Last Post: 04-04-2018, 06:51 AM
  2. porosity problem
    By Andy in forum TIG Welding (GTAW/GTAW-P)
    Replies: 23
    Last Post: 04-18-2015, 04:04 AM
  3. Porosity and dirty looking welds driving me crazy!
    By adamp in forum TIG Welding (GTAW/GTAW-P)
    Replies: 13
    Last Post: 03-28-2014, 03:45 AM
  4. Porosity on cap with 7018 Excalibur
    By Boilermech in forum General Welding Questions
    Replies: 13
    Last Post: 05-09-2013, 09:30 PM
  5. Weld Porosity
    By inthefrey in forum TIG Welding (GTAW/GTAW-P)
    Replies: 14
    Last Post: 04-17-2012, 10:12 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •