    As title specifies

    Recommended tungsten prep

    2% EWLa 1/16th Dia.

    Whats crackin? I am new to the forum and made an intro post in the Intro section.

    I am getting back into welding after 11 years of QC and R&D work with GMAW. Its been many moons since I hit a real lick welding aluminum. I picked up a 255 Ext and so far am impressed with the current DC only use. I have been attempting to run some 1/16th Tungsten and get erratic results with it "balling" up. I initially had some that were sharpened way to sharp and backed off to a 30 degree prep and a blunted point.

    120hz AC, Square wave. 40% EP ~50-60 amps max current.

    Would leaving the electrode square cut be a better prep.

    I did do a search and did not seem to find a related post or topic.

    If there is one then please link and I will read away.

    Regards.

    Jeb.

  2. Default

    Yeah,

    40% EP on the Balance seems a tad much.

    But also check that your torch is in Electrode Negative.

    If you use 1/16" tungsten at a bit higher amperages, I'd switch to 3/32", which is about all I use for 5-210 amps. I'd use 1/8" if I lingered much around 200 or more amps, though.

    Otherwise, a taper on the electrode is best for arc starts.

    What size cup are you using, and how much CFH of Argon?
    Everlast 210 EXT (2015)

    www.youtube.com/newjerusalemtimes

  3. #3

    Default

    Quote Originally Posted by christian View Post
    What size cup are you using, and how much CFH of Argon?
    Number 5

    10-12 CFH

  4. Default

    Yeah,

    That's about right.

    Providing a pic of torch and tungsten newly prepped and also after it's "balled" up from use would help is diagnosing your problem.

    You may just have a fouled tungsten from the puddle or filler touching it.
    Everlast 210 EXT (2015)

    www.youtube.com/newjerusalemtimes

  5. #5

    Default

    I may have not made my self clear.

    How would you prep a 1/16' dia tungsten for AC welding using no more than 50 - 60 Amps.

    Would you leave it square cut and add amperage to obtain a good rounded end?

    Would you put a taper and a blunted end?

    Jeb.

  6. Default

    OK,

    The old method or mentality of balling a "Green" tungsten (with increased AC Balance, briefly changing polarity, or adding amperage) for welding on aluminum with a transformer unit, I think, is a needless holdover when it comes to an inverter machine on aluminum AC welding.

    I think a 1/16" diameter tungsten is small enough that the degree of taper is not so critical, and truncating the tip probably isn't either. But, of course, do as you like. I sometimes do truncate the tip on a 3/32". My dedicated tungsten grinder fixture head (fitted to a Dremel tool) has a semi-fixed angle for the taper, even though it's easy to change it, either way, if I want. I think it's set to 20 degrees for the 3/32' collet right now.

    So, that's what I use for my tungsten prep, AC or DC, with a 3/32. electrode. And if the tungsten tends to start balling on its own, or loses its taper after a while, I'll usually resharpen it then.

    The grinding head that I have, by default, seems to use longer tapers for the smaller diameter tungstens. But, 20 to 30 degrees is all good to me.

    And I never chuck-up the tungsten in a cordless drill like some people do while grinding the tungsten on a belt sander or flap disc, as that could put needless horizontal or diagonal striations in the taper.

    Click image for larger version. 

Name:	Grinder.jpg 
Views:	514 
Size:	87.5 KB 
ID:	14004Click image for larger version. 

Name:	Taper.jpg 
Views:	450 
Size:	98.6 KB 
ID:	14005
    Last edited by christian; 06-04-2020 at 04:08 PM.
    Everlast 210 EXT (2015)

    www.youtube.com/newjerusalemtimes

  7. #7

    Default

    75 amps
    Frequency 120hz
    30% EP

    Click image for larger version. 

Name:	A2797DA6-AA12-473A-805F-9827BA204711.jpg 
Views:	480 
Size:	15.1 KB 
ID:	14006

  8. Default

    Yeah,

    Your setting seems fine, but I'll recommend that you start with any taper, and resharpen after the tip gets balled like that.
    Attached Thumbnails Attached Thumbnails Click image for larger version. 

Name:	Tips.jpg 
Views:	604 
Size:	10.5 KB 
ID:	14007  
    Everlast 210 EXT (2015)

    www.youtube.com/newjerusalemtimes

  9. #9

    Default

    I'd taper it. Don't worry about blunt end. Make it sharp. It will dome itself over that way and provide a better point that if it were blunted.

  10. #10

    Default

    Quote Originally Posted by performance View Post
    I'd taper it. Don't worry about blunt end. Make it sharp. It will dome itself over that way and provide a better point that if it were blunted.
    Thank you.

    Suggested angle? Right now I have them at 30 degrees with a blunt.

  11. #11

    Default

    The grind length should be 2 to 3 times the tungsten diamter. Don't get super concerned about the angle.

Posting Permissions