    I'm using Lincoln NR211MP flux core wire and my welds are very porous. The welds look like I'm using solid wire and ran out of gas. Most of the bead has no slag covering it, only slag in patches. Anybody got any ideas or tips?
    Thanks!

  2. #2
    Join Date
    May 2012
    Location
    Disneyland
    Posts
    2,663

    Default

    What are you welding and with what settings?
    Long arc, short arc, heliarc and in-the-dark!

  3. #3

    Default

    What's the polarity you are using?

  4. Default

    Sounds like you need to change the polarity. flux core polarity is the opposite of hard wire. You should be running 18-19 volts and about 130 imp . That should put you at about 170 amps . If you are welding thinner metal go to about 16-17 volts and you wire speed should be around 100 i.m.p. Its like stick welding in slow motion you will have a lot of control over the weld. You will need to run multiple passes on anything thicker than 1/4 in. I am assuming you are running .045 if you are running smaller wire the settings will be a little different. You can google lincoln nr211 mp and it will have a table with the settings for the various sizes of wire.
    Last edited by TheGary; 06-06-2014 at 11:01 PM.
    Miller 302 gas drive
    millermatic 200 mig
    miller spoolmatic 3 spool gun with 100ft ext.
    2014 Everlast PP60S plasma
    thermal arc 250 GTS inverter
    2016 Everlast 250EX
    miller tig cooler
    2015 Everlast MTS250S
    Miller 30A spool Gun
    Miller xtreme 12VS wire feeder
    Linde CM 85 shape cutter

  5. Default

    Thanks for the replies. Gary, I googled the wire type and found an instruction manual for using this type of wire. That helped a lot. It turns out I was using too much voltage and the welds look MUCH better after I turned the voltage down. The arc seems really short, but the welds look good, so I guess its the right setting.

  6. #6

    Default

    Quote Originally Posted by Chris A View Post
    Thanks for the replies. Gary, I googled the wire type and found an instruction manual for using this type of wire. That helped a lot. It turns out I was using too much voltage and the welds look MUCH better after I turned the voltage down. The arc seems really short, but the welds look good, so I guess its the right setting.
    What polarity are you using ?
    2013 250EX : SSC Pedal : I-MIG 250P 20' Profax gun : Power Plasma 60 p80 torch : 3M Speedglas 9100XX : Evolution Rage 3 DB cold saw

  7. Default

    My gun is hooked to negative.

Similar Threads

  1. HF Flux Core?
    By Elantramax1 in forum General Welding Questions
    Replies: 7
    Last Post: 10-27-2014, 09:07 PM
  2. Flux Core?
    By Elantramax1 in forum General Welding Questions
    Replies: 57
    Last Post: 09-29-2014, 12:25 PM
  3. Imig200 flux core welding questions
    By sw2x in forum MIG Welding (GMAW/GMAW-P/FCAW)
    Replies: 17
    Last Post: 03-30-2013, 10:24 AM
  4. Gas vs flux core
    By MigPlazArc in forum MIG Welding (GMAW/GMAW-P/FCAW)
    Replies: 17
    Last Post: 10-06-2011, 03:11 AM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •