Thread: 2" sch 80 tig root 7018 cap 6g test help

  1. #21

    Default

    Quote Originally Posted by Boilermech View Post
    Here is my last try on the root pass for tonight. Please criticize, thanks.
    Attachment 9958
    Attachment 9959
    Attachment 9960

    Thanks again everyone for any and all help.
    Forgot to mention this is a tight 3/32 gap, 3/32 70S6, 3/32 tungsten, lay wire technique, 90 amps and 8 lpm gas.
    Now, try dipping. OK, I see something...and have thought of something else. The sides aren't tied in, and it looks like your ripple separation is too big...that's still sign you are using too much amps and moving too fast....90 amps is way too much as evidence by the overreinforcement inside. While the weld inside should suck back it should be fairly flat, or you'll get a restriction in the flow.

    Try, wiggling the torch,(walking the cup) about as fast as you can, or freehand the torch so it is running from side to about 3 times a second.

    What you have in the pipe from what I was taught and know, is way too m uch reinforcement still all the way around. Too much filler at too many amps causes this. Again, no suck back, but the backside should be flat and actually, if done right won't be but about 3/32 wide.

  2. Default

    Ok Mark I done one with 70 amps and here are pics of it.
    Click image for larger version. 

Name:	uploadfromtaptalk1367124928540.jpg 
Views:	911 
Size:	115.5 KB 
ID:	9969
    Click image for larger version. 

Name:	uploadfromtaptalk1367124956297.jpg 
Views:	646 
Size:	42.6 KB 
ID:	9970
    Click image for larger version. 

Name:	uploadfromtaptalk1367124983878.jpg 
Views:	585 
Size:	70.2 KB 
ID:	9971

  3. #23

    Default

    Best one yet. Still a little too much inside reinforcement in a couple spots, and maybe a little under, but that's not bad. The bead contour looks a LOT better on the outside.

  4. Default

    Figured out why I couldn't get the root in all the way. I was keeping my tungsten in the cup to far and couldn't reach the end of the bevels to use the arc force to push it in. I was breaking down the walls but I was holding the tungsten back and it was making the filler wire bridge over the bevel and not pushing it to the inside. Thank you Mark and everyone else for your help. Finally getting it and now I'm not to nervous about the test. I'll let you all know how it goes after the 17th of June.

  5. #25

    Default

    Sounds like you've made some great progress. That is what I like about this forum, it has some great people who are willing to help out. I also like the fact that Everlast staff are both knowledgeable and active on this forum.

  6. Default

    Quote Originally Posted by Mr120 View Post
    Sounds like you've made some great progress. That is what I like about this forum, it has some great people who are willing to help out. I also like the fact that Everlast staff are both knowledgeable and active on this forum.
    I talked with Mark on the phone the other day and he pointed me in the right direction. Along with the tips from everyone else on here I just passed my tig root 7018 cap bend test tonight at school. My instructor told me that if I keep it up then the actual test shouldn't be a problem. I cant wait till the 17th to get my state license out of the way. This was the root that passed the bend test. Sorry didn't get a pic of the inside until after the hot pass and it wasn't as pretty then, lol. But it was in all the way.

    Click image for larger version. 

Name:	uploadfromtaptalk1367544343948.jpg 
Views:	681 
Size:	38.0 KB 
ID:	10005

    Sent from my XT901 using Tapatalk 2

  7. #27

    Default

    Fantastic news. Keep practicing and I hope the 17th will be a breeze for you!

Similar Threads

  1. tig root 2G lay wire technique?
    By GaveUpOnTV in forum General Welding Questions
    Replies: 7
    Last Post: 08-08-2016, 01:30 PM
  2. Anyone get "give away" electrodes other than 7018 scrap?
    By EchoSixMike in forum Stick Welding (SMAW)
    Replies: 15
    Last Post: 06-12-2012, 12:45 PM
  3. aws weld cert G6 open root
    By jojobead in forum General Welder Questions
    Replies: 1
    Last Post: 07-23-2011, 02:51 AM
  4. "Test pipe" welding
    By jakeru in forum Other Custom Fabrications
    Replies: 3
    Last Post: 03-23-2011, 03:27 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •