  1. Default 1/8 alum 250 ex settings

    I had a class two years ago from HTP welding. They set up the 201 machine and I was welding with there supervision. Can you give me a base set up I will figure out the rest. I could use help from a pro. I want to use the pulse setting and weld a box.
    Last edited by rx7nos; 02-13-2010 at 12:33 AM.

  2. #2

    Default

    I can tell you where I would start if I had a little more information.

    First questions I have. What type filler? You are running straight argon? What type electrode (tungsten type)? Do you have a fresh stainless steel brush to clean the parts you are going to weld?

    A lot of factors for aluminum.

    If you want to PM me a phone number and good time to call (and timezone), I can give you a call tomorrow (Saturday).

    Once you get dialed in, it would be nice if you post your results and photos.

    There is a good intro on the web on weldingtipsandtricks.com.

    http://www.everlastgenerators.com/fo...gtipsandtricks

    Off to see part 3 and 4 as I did not know they where out.

    See part 2 for general aluminum settings, but the questions I asked are still key for a good weld.
    Mike R.
    Email: admineverlast@everlastwelders.com
    www.everlastgenerators.com
    www.everlastwelders.com
    877-755-9353 x203
    M-F 12 - 7PM PST
    FYI: PP50, PP80, IMIG-200, IMIG-250P, 210EXT and 255EXT.

  3. #3

    Default

    I have no PM from you. I think my point is you asked a question and you gave no info/details (or not all of them).

    I am tech support for our units. No two people weld the same. But I will do that offline with you if you like.

    I can help you with the welding and you can post your results?
    Mike R.
    Email: admineverlast@everlastwelders.com
    www.everlastgenerators.com
    www.everlastwelders.com
    877-755-9353 x203
    M-F 12 - 7PM PST
    FYI: PP50, PP80, IMIG-200, IMIG-250P, 210EXT and 255EXT.

  4. Default

    here is a basic set up for me....150-165 amp-ac freq8.1-ac bal3.1, hope that gets ya in the right direction.

Similar Threads

  1. pro 205 alum ??
    By braveops in forum Multi-Process Units (TIG,Stick,Plasma/MIG,TIG,Stick Combo units)
    Replies: 2
    Last Post: 01-28-2016, 11:27 PM
  2. I-Mig 205P Spoolgun Alum. welding First Time
    By Kempy in forum MIG Welding (GMAW/GMAW-P/FCAW)
    Replies: 18
    Last Post: 03-03-2013, 09:08 PM
  3. a little DCEN on some 1/8 alum
    By Wookie in forum TIG Welding (GTAW/GTAW-P)
    Replies: 1
    Last Post: 05-04-2011, 01:47 AM
  4. ac tig settings
    By iil in forum TIG Welding (GTAW/GTAW-P)
    Replies: 7
    Last Post: 12-24-2010, 01:46 AM
  5. welding alum with poweritig250
    By mrmuddy76 in forum General Welding Questions
    Replies: 15
    Last Post: 11-30-2009, 01:45 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •