    If you were using 5356 filler and your new bottle contained some CO2, the magnesium in the filler will react with CO2 forming magnesium oxide and carbon.
    2013 250EX : SSC Pedal : I-MIG 250P 20' Profax gun : Power Plasma 60 p80 torch : 3M Speedglas 9100XX : Evolution Rage 3 DB cold saw

  2. Default

    i only got 4043, and i tried rods from 3 different batches earlier, no luck, i'll be sure to give you guys an update when i get the new bottle and try it out.

  3. #3

    Default

    bad tank of gas . i have got 2 or 3 bottles of bad gas argon and co2 and argon mix . I asked Jessie from A&B gas he tells me its the guys being lazy when checking and filling tank he says the killer is having air or oxygen in the tank before filling .he say happens when welder run a tank empty and after removing welding gauges leaves tank valve open condensation forms and air gets in tank , the fill guy when see a tank with a valve open or empty totally is suppose to purge tank with argon and evac tank before refilling , he just fired one of his guys because it cost money for bad gas fills and dosnt look good for his business. think i will make a dryer for my argon hose lol
    Last edited by Rodsmachineshop; 08-24-2012 at 02:09 AM.
    EVERLAST 250 EX , EVERLAST I-MIG 205 , EVERLAST spool gun NOW have 2 EVERLAST POWER PLASMA 50 plasma cutter's , LINCOLN 175HD MIG WELDER , VICTOR TORCH SET and many more tools to many to list

  4. #4

    Default

    Quote Originally Posted by Rodsmachineshop View Post
    bad tank of gas . i have got 2 or 3 bottles of bad gas argon and co2 and argon mix . I asked Jessie from A&B gas he tells me its the guys being lazy when checking and filling tank he says the killer is having air or oxygen in the tank before filling .he say happens when welder run a tank empty and after removing welding gauges leaves tank valve open condensation forms and air gets in tank , the fill guy when see a tank with a valve open or empty totally is suppose to purge tank with argon and evac tank before refilling , he just fired one of his guys because it cost money for bad gas fills and dosnt look good for his business. think i will make a dryer for my argon hose lol
    I think you hit it Rod. Looks like air with the black. There is no fan blowing is there? I posted the video in the tech area some time ago, have not made on yet but can't hurt. I did make a kitty litter crystals filter for the compressor though.

    But yea, looks like air getting in the mix somehow.
    Mike R.
    Email: admineverlast@everlastwelders.com
    www.everlastgenerators.com
    www.everlastwelders.com
    877-755-9353 x203
    M-F 12 - 7PM PST
    FYI: PP50, PP80, IMIG-200, IMIG-250P, 210EXT and 255EXT.

  5. Default

    Finally got a new tank and things seem to be back to normal, i only had time to try a couple beads, but the weld pool was clean and not black soot and the cleaning was back. I will update with some after pics when i get a chance.

  6. #6

    Default

    Quote Originally Posted by Infidel View Post
    Finally got a new tank and things seem to be back to normal, i only had time to try a couple beads, but the weld pool was clean and not black soot and the cleaning was back. I will update with some after pics when i get a chance.
    Interesting... There have been a few posts lately with people having a contaminated tank. You would think their would be a little more quality control.
    Shade tree MIG welder.
    Now a Shade tree TIG welder.

  7. #7

    Default

    Quote Originally Posted by Brian Ski View Post
    Interesting... There have been a few posts lately with people having a contaminated tank. You would think their would be a little more quality control.
    Every year people seem to get a little more lazy and a little more greedy... both are highly contagious in the workplace.
    2013 250EX : SSC Pedal : I-MIG 250P 20' Profax gun : Power Plasma 60 p80 torch : 3M Speedglas 9100XX : Evolution Rage 3 DB cold saw

Similar Threads

  1. Cleaning dirty aluminum
    By JohnT in forum TIG Welding (GTAW/GTAW-P)
    Replies: 7
    Last Post: 11-08-2014, 11:53 AM
  2. AC balance & cleaning
    By broberts5 in forum TIG Welding (GTAW/GTAW-P)
    Replies: 18
    Last Post: 01-15-2014, 11:34 PM
  3. Cleaning of the welder itself
    By Jules The Great in forum TIG Welding (GTAW/GTAW-P)
    Replies: 7
    Last Post: 04-20-2012, 08:19 PM
  4. Spring Cleaning...
    By wruehl in forum Personal Projects (no welder required)
    Replies: 13
    Last Post: 04-29-2011, 12:18 AM
  5. Cleaning - How much is needed.
    By sschefer in forum TIG Welding (GTAW/GTAW-P)
    Replies: 5
    Last Post: 12-21-2010, 05:27 AM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •