    Post Weld Porosity

    Greetings all!

    I started welding up the new cart this week and found I'm having problems with weld porosity.
    The material is 1/8" wall by 1" square mild steel tubing. All basic butt joints - nothing fancy.

    Using 3/32, 2% Lanth. electrodes.
    Filler - 3/32 ER70S-2
    Amps set between 80 and 90.
    Material is cleaned with flap disk.
    Pre and post flow set to 5 and 8 respectively. I'll start the weld, puddle forms, add filler and start moving. About 7-8 second in, I SEE THE PUDDLE START TO BOIL BEHIND ME!

    Tried reducing amps
    increasing flow rate - reducing rate. slowing down, speeding up
    went to larger cup size.

    Arrrg!!!!

    Used almost a whole 60CF bottle of gas this afternoon trying to figure this
    out and,............


    Wait for it....


    I'm absolutely sure I doing something stupid.


    Recommendations welcome. THANKS!
    Last edited by inthefrey; 04-14-2012 at 10:25 PM.

  2. #2

    Default

    How much argon flow do you have?

    The puddle should be frozen pretty much as soon as you move.
    Everlast 200DX
    Everlast PT185
    Shoptask 3-in-1 (not currently in my garage, but I own it...)

    Any day on a motorcycle like this that ends just needing parts and labor is a good day.
    4.82, 158.67mph 1/8th mile 7.350, 200.35mph 1/4 mile

  3. #3

    Default

    Just a newbie here... So take my advice with a grain of salt... Was told to use tungsten rod about 1/2 the thickness of the material. Try a 1/16" rod and see if it concentrates the heat better.

    Sounds like air getting to the weld before it has completely cooled. So maybe to hot and moving faster. The smaller rod may help.

    Will have to keep watching and see what the pros say.
    Shade tree MIG welder.
    Now a Shade tree TIG welder.

  4. #4

    Default

    I've had this happen one time and that one time I was Extremely hot just trying out the new welder settings.

    Maybe try a larger cup size to get better gas coverage.
    PowerTig 250EX
    Power I-MIG 200
    Power Plasma 50
    It's what you learn, After you know it all, that counts!

  5. #5
    Join Date
    Mar 2012
    Location
    Western Pennsylvania
    Posts
    63

    Default

    Quote Originally Posted by sportbike View Post
    How much argon flow do you have?

    The puddle should be frozen pretty much as soon as you move.
    Using approximately 15CFH - acording to the gauge that came with the PP 205, about 7.5 (CFH x 0.472). Too much? Not enough?

  6. Default

    Quote Originally Posted by inthefrey View Post
    Using approximately 15CFH - acording to the gauge that came with the PP 205, about 7.5 (CFH x 0.472). Too much? Not enough?
    I have the PP205 too and sounds reasonable, especially with your pre and post flow settings. I agree with CGINC, try a larger cup with a gas saver lens. In my opinion it concentrates the argon in a more consistent manner. Once I did this, I was able to dial the argon flow back to 5 lpm and used pre and post flow accordingly.

  7. #7
    Join Date
    Mar 2012
    Location
    Western Pennsylvania
    Posts
    63

    Default

    Well, I may have figured it out.

    I believe I have found my smoking gun.....Guess what kind of hose I replaced my old hose with because I thought I was getting a good deal?! They were only $9.99 for a 25' length!

    http://forum.weldingtipsandtricks.co...php?f=5&t=1022

    Fixed the link. I dunno?!


    I guess I'll be at HD tomorrow - spending some money on new tank lines. Going to give it a try and see what happens.
    Last edited by inthefrey; 04-16-2012 at 10:07 PM.

  8. #8
    Join Date
    Oct 2010
    Location
    Northern Virginia
    Posts
    1,323

    Default

    I get an error when I click that link... what happened? The hose failed on you?
    DaveO
    Oxweld oxy acet gear
    IMIG 200
    PowerTIG 210 EXT... Amazing!

  9. #9

    Default

    Quote Originally Posted by DaveO View Post
    I get an error when I click that link... what happened? The hose failed on you?
    I found the thread...

    http://forum.weldingtipsandtricks.co...php?f=5&t=1022

    Crappy hose...

    Interesting. The link gets altered... Try this if the above link does not work. Might have to cut and paste it.

    //forum.weldingtipsandtricks.com/viewtopic.php?f=5&t=1022
    Last edited by Brian Ski; 04-16-2012 at 08:52 PM.
    Shade tree MIG welder.
    Now a Shade tree TIG welder.

  10. #10
    Join Date
    Mar 2012
    Location
    Western Pennsylvania
    Posts
    63

    Default

    Quote Originally Posted by Brian Ski View Post
    I found the thread...

    http://forum.weldingtipsandtricks.co...php?f=5&t=1022

    Crappy hose...

    Interesting. The link gets altered... Try this if the above link does not work. Might have to cut and paste it.

    //forum.weldingtipsandtricks.com/viewtopic.php?f=5&t=1022


    So, according to the info above, the cheap lines are bleeding chems, gases or whatever into the argon. I'll be replacing the lines tonight. I'll let everyone know if it helped or cured the problem.
    Last edited by inthefrey; 04-16-2012 at 10:17 PM.

  11. #11

    Default

    Quote Originally Posted by inthefrey View Post
    So, according to the info above, the cheap lines are bleeding chems, gases or whatever into the argon. I'll be replacing the lines tonight. I'll let everyone know if it helped or cured the problem.
    Are your hoses polyethelyne (thin simi-rigid)Click image for larger version. 

Name:	mazzer_recoil.jpg 
Views:	593 
Size:	19.8 KB 
ID:	6279 or PVC (similar to rubber air hose) ? Click image for larger version. 

Name:	41E6UHkyVXL._SL500_AA300_.jpg 
Views:	547 
Size:	15.2 KB 
ID:	6280 I use PVC air hose with no problems. The clear braided hose that comes with the welders is also PVC.
    Last edited by zoama; 04-16-2012 at 10:42 PM.
    2013 250EX : SSC Pedal : I-MIG 250P 20' Profax gun : Power Plasma 60 p80 torch : 3M Speedglas 9100XX : Evolution Rage 3 DB cold saw

  12. #12
    Join Date
    Mar 2012
    Location
    Western Pennsylvania
    Posts
    63

    Default

    Quote Originally Posted by zoama585 View Post
    Are your hoses polyethelyne (thin simi-rigid)Click image for larger version. 

Name:	mazzer_recoil.jpg 
Views:	593 
Size:	19.8 KB 
ID:	6279 or PVC (similar to rubber air hose) ? Click image for larger version. 

Name:	41E6UHkyVXL._SL500_AA300_.jpg 
Views:	547 
Size:	15.2 KB 
ID:	6280 I use PVC air hose with no problems. The clear braided hose that comes with the welders is also PVC.
    Hi Zoama. They are PVC. However, they have got to be the stiffest hoses I've ever used. If it's cold, forget about it! Like I said, I got them on the cheap so, no great loss in giving this a try. Actualy, the one I'm replacing looks like the blue one! In any case, I'll have an extra now.

    Now, all this may be an excersize in folly and I just got a bad tank of gas. I get the tank filled tomorrow - from a different dealer.

    I'll get it figured out.

    Thanks!
    Last edited by inthefrey; 04-17-2012 at 02:54 AM.

  13. #13
    Join Date
    Mar 2012
    Location
    Remote S. Idaho
    Posts
    53

    Default

    Tubing is sometimes tough because the heated air inside will blow out through the puddle.
    Argon is heavier than air--when welding up tubing, try to have the open end of the tube up. Before welding the joint, trip the torch with the post flow set on 20 seconds or so and fill the tube with argon, then weld. If the tubing has to be open end down, always stuff a paper towel in the bottom to kill the 'chimney' effect that blows air on the back side of the puddle.
    There is no safe direction to point an unsafe gun.
    PowerPro 205
    Hobart 250HF
    Powcon 300ST
    gas stuff
    14x60 Hercules Ajax lathe
    Gorton I-22 MastrMil
    Landis 6x18 surface grinder
    20" Powermatic bandsaw
    Ancient, big drill press
    350 pound anvil and a bunch of hammers
    If I can't fix it I can make it.....unrecognizable.

  14. #14
    Join Date
    Mar 2012
    Location
    Western Pennsylvania
    Posts
    63

    Default

    Quote Originally Posted by JBnID View Post
    Tubing is sometimes tough because the heated air inside will blow out through the puddle.
    Argon is heavier than air--when welding up tubing, try to have the open end of the tube up. Before welding the joint, trip the torch with the post flow set on 20 seconds or so and fill the tube with argon, then weld. If the tubing has to be open end down, always stuff a paper towel in the bottom to kill the 'chimney' effect that blows air on the back side of the puddle.
    This is a GREAT tip! Never though of this but it makes complete sense. THANKS!

  15. #15

    Default

    Heated air only blows through the puddle on tubing when you make the last weld to seal it. Always back purge stainless but on steel or aluminum you can leave a small opening on the last weld, then come back and close it when cooled without purging.
    2013 250EX : SSC Pedal : I-MIG 250P 20' Profax gun : Power Plasma 60 p80 torch : 3M Speedglas 9100XX : Evolution Rage 3 DB cold saw

Similar Threads

  1. New 185dv owner with a porosity issue
    By Deep Six in forum TIG Welding (GTAW/GTAW-P)
    Replies: 40
    Last Post: 04-04-2018, 06:51 AM
  2. porosity problem
    By Andy in forum TIG Welding (GTAW/GTAW-P)
    Replies: 23
    Last Post: 04-18-2015, 04:04 AM
  3. Porosity on cap with 7018 Excalibur
    By Boilermech in forum General Welding Questions
    Replies: 13
    Last Post: 05-09-2013, 09:30 PM
  4. PowerPro 205 - first BIG welds - porosity issues resolved
    By inthefrey in forum TIG Welding (GTAW/GTAW-P)
    Replies: 4
    Last Post: 04-22-2012, 12:27 AM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •