Thread: Alternative Tungsten Alloys (Ceriated, Zirconiated, Lanthanated, Rare Earth, etc.)

  1. #21

    Default

    I am still absolutely loving the Lanthanated tungsten for aluminum welding. Here's a couple of aluminum welds i did on some tubing structure for a custom touring motorcycle that i'm building.

    -------------------------------------------
    Spike Customs, Inc.
    Fresno, CA 93727
    ph- 559-549-RIDE(7433)
    -------------------------------------------
    -Follow me on twitter!-

  2. #22

    Default

    I like 2% lanthanated I have to order them from diamond ground but they hold up alot better than 1.5% lanthanated. They are $24 a box for 3/16th and $14 for 1/16th Nice work by the way.
    Everlast PowerTig 250EX
    Everlast PowerCool 300
    Everlast PowerPlasma 70
    Lincoln Powermig 215
    Magnum SG Spool Gun
    Don't jump on my Gomba

  3. #23

    Default

    Quote Originally Posted by Cippee View Post
    I like 2% lanthanated I have to order them from diamond ground but they hold up alot better than 1.5% lanthanated. They are $24 a box for 3/16th and $14 for 1/16th Nice work by the way.
    its on here somewhere else, but try weldingcity.com. they dont have 2%lath but the 1.5 are dirt cheap. 8.90 for ten 1/16"... also considering at my LWS a ten padck of 2% thoriated 1/8" was 100$!!!, weldingcity was only 25.... even with shipping i still save a lot of money
    Journeyman welder
    250EX
    Power plasma 60
    horizontal band saw
    Miller digital elite 'wicked' lid

  4. Default

    Spike,

    For a test, after grinding your tungsten to a sharp tip, put a .050 diameter flat on the tip for aluminum. It gives me a more consistent width of weld and a much flatter weld on aluminum.

  5. #25

    Default

    Quote Originally Posted by srp View Post
    Spike,

    For a test, after grinding your tungsten to a sharp tip, put a .050 diameter flat on the tip for aluminum. It gives me a more consistent width of weld and a much flatter weld on aluminum.
    I don't sharpen my tungsten to a complete point unless I'm doing low amperage work, otherwise it just burns the tip off anyway. I found that just making the tungsten "less dull" target than "sharp" works best for me when welding stuff like the 5/16" aluminum in the last picture.
    -------------------------------------------
    Spike Customs, Inc.
    Fresno, CA 93727
    ph- 559-549-RIDE(7433)
    -------------------------------------------
    -Follow me on twitter!-

  6. #26

    Default

    1.5% lanthanated compared to 2% lanthanated are a big difference is performance. Trust me 2%.is not comparison to 1.5%. You wouldn't think .5% would make alot of difference but it does. To see a test of them all check this out http://www.weldingtipsandtricks.com/...odes-gtaw.html
    Everlast PowerTig 250EX
    Everlast PowerCool 300
    Everlast PowerPlasma 70
    Lincoln Powermig 215
    Magnum SG Spool Gun
    Don't jump on my Gomba

  7. #27

    Default

    alright, so... with the lanthanated tungstens, i've figured out that it works best for me if i grind a *much* longer taper onto the tungsten than i normally would with thoriated with DC current (about 2x the length), and then thinking about what SRP said, i ground a little flat onto the end of the tungsten, for the lower current sheetmetal aluminum work it makes the welding puddle much more precise and easier to control... for the higher current work, it doesn't seem to make as much difference.
    I am surprised that the extra long taper on the tungsten still doesn't roll up into a ball even at 160 amps.
    -------------------------------------------
    Spike Customs, Inc.
    Fresno, CA 93727
    ph- 559-549-RIDE(7433)
    -------------------------------------------
    -Follow me on twitter!-

  8. #28

    Default

    Here is an aluminum weld i did on a sheetmetal project that i'm working on. This is with the elongated lanthanated tungsten (3/32" electrode) on some .063" 5052 sheet.
    I think i should have put a ruler in the picture to show the scale. The piece in the pictre is only 1.5" wide from, making the weld beads less than 1/4" wide. (the threads are only 5/16", if that helps)

    -------------------------------------------
    Spike Customs, Inc.
    Fresno, CA 93727
    ph- 559-549-RIDE(7433)
    -------------------------------------------
    -Follow me on twitter!-

  9. #29
    Join Date
    Dec 2009
    Location
    Greater Seattle, WA
    Posts
    813

    Default

    After using the same, 2% lanthanted 1/16" tungsten for a reeeeeally long time, it was finally getting a little too short to use any much longer, and so I just grabbed a piece of 1.5% lanthanted 1/16" tungsten that I had handy, laying around. I was surprised that I noticed a definite difference of the 1.5% versus the 2%! The 1.5% has more of a tendency to grow the "protrusions" than the 2%.... especially if you keep welding after an aluminum puddle dip. The 2% seems to handle welding after an aluminum puddle dip much better than the 1.5%. The 1.5% grows fairly large "protrusions" fairly quickly. They don't grow as large or as fast on the 2%. I like the 2% lanthanated better; it keeps it point better. It can put up with a LOT of heat and current too. Both are excellent arc starters (especially if bathed in pure argon... it's pure blissfully easy arc starts.)

    By the way, I really like being able to just twist the footpedal current knob from 200A to 100A, and simply shut off the Helium gas valve, and have a setup for welding very delicate, thin parts, and then, just undo those two changes, and have a really powerful setup able to melt very thick parts and good penetration. I have rarely ever changed my tungsten from 1/16" since getting the Helium mix... I'd rather just turn on or off the Helium than bother running higher amps on pure argon and force having to swap out the torch parts to put in a 3/32" tungsten. I think the 2% lanthanated (instead of just 1/5%) may be small, but important part of that equation also (for getting that last bit of possible current and heat out of the 1/16" tungsten tip, without it quickly forming the multiple protrusions.)
    '13 Everlast 255EXT
    '07 Everlast Super200P

Similar Threads

  1. Does 250ex require additional earth ??
    By brownchoclit in forum TIG Welding (GTAW/GTAW-P)
    Replies: 2
    Last Post: 07-10-2014, 02:43 AM
  2. Cooler alternative
    By azsprint6 in forum Tips & Tricks, Custom Tools, Safety, Ideas and Reviews.
    Replies: 7
    Last Post: 01-19-2014, 10:33 PM
  3. TIG 200DX Alternative Pedal Option
    By compression in forum TIG Welding (GTAW/GTAW-P)
    Replies: 11
    Last Post: 04-18-2012, 07:12 PM
  4. Pure & Zirconiated, Why Not?
    By redbeard in forum TIG Welding (GTAW/GTAW-P)
    Replies: 13
    Last Post: 12-20-2011, 05:47 AM
  5. Alternative tig torch selecton for pp205
    By rodjava in forum Multi-Process Units (TIG,Stick,Plasma/MIG,TIG,Stick Combo units)
    Replies: 3
    Last Post: 01-04-2011, 08:24 PM

Tags for this Thread

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •