    Default O Holey Weld

    Well, OK maybe it's a bit early for a Christmas pun, but...

    This is the first time I have ever had a weld that wound up with holes in it and I am wondering what caused it. The rod was 1/8 7018 at about 120A on the buzzbox. I did notice that the worst spot is where I experimented and got really perpendicular, but even where I kept a lower angle it still is a bit porous.

    Click image for larger version. 

Name:	DSCN0657.jpg 
Views:	541 
Size:	143.5 KB 
ID:	3373Click image for larger version. 

Name:	DSCN0659.jpg 
Views:	540 
Size:	122.2 KB 
ID:	3374Click image for larger version. 

Name:	DSCN0662.jpg 
Views:	536 
Size:	121.9 KB 
ID:	3375
    Penncrest Buzzbox - Infinite amp control! Man the 70's were good.
    Everlast Powerplasma 60 - Reliable unit, cuts well.
    Everlast i-MIG 250P w/spoolgun - Really smooth, plenty of cajones.
    Everlast 250EXT - Sometimes it just takes a kick in the balls...
    Everlast 255EXT - Just started playing

  2. #2

    Default

    That's really interesting how it blew out like that.

    1> Have you tried running these same rods in the same exact way on a different piece of like flat stock?

    2> How old are your 7018's and are they dry? - I've seen blow out like that when a guy had moisture in his rods.

    3> You might try 7018AC's to see if it improves any. - Since you are using an AC power source.
    I Love Plasma and rolleye's at the costly addiction of MAPPgasoron's.

    http://brothers2woodworking.webstarts.com/

    Everlast Plasma cutter Power Plasma 50
    Everlast PowerArc 200 ~ Happily Married To That gutsy babe, git'er dun.


    Wishlist: Free consumables, Small TIG maybe Alex, when you have overstock give me ring!

  3. #3

    Default

    i like to call those worms, but really its porosity. you need to CLEAN your metal before you weld it. especially with 7018. 6010 you might have gotten away with it. with that flat weld, you should have about a 45-60 rod angle.
    Journeyman welder
    250EX
    Power plasma 60
    horizontal band saw
    Miller digital elite 'wicked' lid

  4. #4

    Default

    What I see is fairly good. The holes are in the slag. Too long of an arc/too cool is part of the problem if the slag holds fast like that. Go watch our powerarc video online and you'll see an example of how slag should pop right off.

  5. #5
    Join Date
    Mar 2011
    Location
    Eastern Oregon
    Posts
    681

    Default

    That is actually one of the few welds I've made that I'm not embarrassed to show in public. It is also the first one I've done that required enough fill that I actually got to play in the puddle.

    Believe it or not, I did run the grinder down the trench after I tacked it, but maybe the little bit at the bottom I couldn't reach was enough to hose me.

    Good to know about arc length and slag adhesion, I had noticed that sometimes it pops easily and other times not but never figured out why.

    Just for grins, I ran the last half of the rod on the nastiest piece of steel I could find, and came up with one of the most consistent beads I have ever laid down. Go figure.

    Click image for larger version. 

Name:	DSCN0678.jpg 
Views:	535 
Size:	88.5 KB 
ID:	3381
    Penncrest Buzzbox - Infinite amp control! Man the 70's were good.
    Everlast Powerplasma 60 - Reliable unit, cuts well.
    Everlast i-MIG 250P w/spoolgun - Really smooth, plenty of cajones.
    Everlast 250EXT - Sometimes it just takes a kick in the balls...
    Everlast 255EXT - Just started playing

  6. #6

    Default

    What brand of rod are you running? Hobart 7018s seem to be cantankerous at times, especially trying to run them on AC.
    Everlast lx225
    Hobart Handler 210 with spool gun
    Hobart Stickmate LX
    Thermal Arc 400GMS
    40 amp Northern Tools plasma torch
    130 chicago electric tig welder
    90 amp chicago electric flux mig
    10"-22" Grizzly lathe
    15"-5.5" Grizzly vertical end mill

    In need of nice TIG machine. drooling over PowerTig 250ex

  7. #7
    Join Date
    Mar 2011
    Location
    Eastern Oregon
    Posts
    681

    Default

    I think they were Lincolns, but it's been a long time since I got them and I didn't save the box label. Whatever they are, they were the reason I fell in love with 7018, easiest rod I ever used.

    I see what you mean about the Hobarts, just cracked a new box of 418 and couldn't even hold an arc , granted, it wasn't a very nice piece to be running a bead on, but I'm used to being able to throw a good arc on just about anything with the batch I'm working on now. Guess I'll have to get that TIG now just so I can burn the new box of rod.
    Penncrest Buzzbox - Infinite amp control! Man the 70's were good.
    Everlast Powerplasma 60 - Reliable unit, cuts well.
    Everlast i-MIG 250P w/spoolgun - Really smooth, plenty of cajones.
    Everlast 250EXT - Sometimes it just takes a kick in the balls...
    Everlast 255EXT - Just started playing

  8. #8

    Default

    I would play with your temp settings, when the temps are right the slag tends to chip away pretty easy. That may help with you purosity as well.
    Lincoln Eagle Engine Drive
    Everlast MTS 250
    Everlast Power Tig 225lx
    HTP Mig 2400
    Everlast Power Plasma 60C --> Just need to finish my CNC Plasma Table!
    Miller Spectrum 375 Extreme Plasma cutter
    Victor cutting torch
    HF 20 Ton Shop Press
    HF 4x6 Band Saw
    HF Air Compressor
    Northern Tool Drill Press


    www.murphywelding.com

  9. #9

    Default

    It looks like porosity at the tie-ins, to me. if you don't get a new rod going before the slag puddle cools, you have to chip/grind it out, or you get porosity like this. it's less of a worry with 6010/6011, they leave thinner slag and burn out more crap than 7018.

    +1 on the slag indicator of heat, too. if you watch a couple of Jody's vids (at weldingtipsandtricks.com), there's at least one that he chips the slag off with the butt end of another rod. that's how easy it should come off. this vid @ about 8:15 http://www.weldingtipsandtricks.com/stick-welding.html

    [edit:] I just noticed that Jody's 'backstepping' technique is tieing into cold slag. he doesn't seem to be getting porosity, but I've had issues with it before.
    Last edited by ogorir; 10-11-2011 at 03:08 PM.
    McGuire Irvine
    Crow Motor Co.

    Lincoln powermig 225 (work)

  10. #10

    Default

    Quote Originally Posted by ogorir View Post
    It looks like porosity at the tie-ins, to me. if you don't get a new rod going before the slag puddle cools, you have to chip/grind it out, or you get porosity like this. it's less of a worry with 6010/6011, they leave thinner slag and burn out more crap than 7018.

    +1 on the slag indicator of heat, too. if you watch a couple of Jody's vids (at weldingtipsandtricks.com), there's at least one that he chips the slag off with the butt end of another rod. that's how easy it should come off. this vid @ about 8:15 http://www.weldingtipsandtricks.com/stick-welding.html

    [edit:] I just noticed that Jody's 'backstepping' technique is tieing into cold slag. he doesn't seem to be getting porosity, but I've had issues with it before.
    you can tie in without cleaning the slag off, but you have to be careful as ya, you can get porosity, slag inclusions and other crap in your weld. usually if im running a few beads or whatever and my base metal is still hot, i usually wont worry about it. i dont allow anything to really cool, just pull out the burnt rod, slap a new one in and keep going. i also run fairly hot with 7018 all the time so it helps to burn that crud out.
    Journeyman welder
    250EX
    Power plasma 60
    horizontal band saw
    Miller digital elite 'wicked' lid

  11. #11
    Join Date
    Oct 2011
    Location
    Litchfield Park, AZ
    Posts
    370

    Default

    redbeard,

    You should pull out a grinder and clean up the material before welding. If you are on clean metal you will have much better luck keeping a consistent ark. Also, cleaning off slag will help with the weld. You are not performing welds that will be radio-graphed but if you do not clean off the slag on a radio-graphed weld it will fail and is not the best practice if you ever make critical welds (e.g. fix a trailer).

    DVA
    Miller 252
    PowerTig 250 EXT
    Evolution Rage 2
    48X6 inch Belt Sander w/ 9 inch Disk Sander
    ...

  12. #12
    Join Date
    Mar 2011
    Location
    Eastern Oregon
    Posts
    681

    Default

    Quote Originally Posted by ogorir View Post
    It looks like porosity at the tie-ins, to me. if you don't get a new rod going before the slag puddle cools, you have to chip/grind it out, or you get porosity like this. it's less of a worry with 6010/6011, they leave thinner slag and burn out more crap than 7018.
    Good catch that it is mostly at the tie-ins, there are a few odd ones out in the middle, but I hadn't really thought about the cold slag aspect. Most of the beads I've run are usually shorter than a full stick, so I haven't had to deal with that.
    Penncrest Buzzbox - Infinite amp control! Man the 70's were good.
    Everlast Powerplasma 60 - Reliable unit, cuts well.
    Everlast i-MIG 250P w/spoolgun - Really smooth, plenty of cajones.
    Everlast 250EXT - Sometimes it just takes a kick in the balls...
    Everlast 255EXT - Just started playing

Similar Threads

  1. Adapter for weld tec
    By Steves1967 in forum TIG Welding (GTAW/GTAW-P)
    Replies: 5
    Last Post: 01-06-2018, 04:37 PM
  2. My very first weld....ever.
    By CharlzO in forum Welding Projects and Pictures
    Replies: 2
    Last Post: 11-17-2014, 04:18 PM
  3. How to weld TALL weld beads on 1.6mm thick Aluminum Tube?
    By Welderooni in forum TIG Welding (GTAW/GTAW-P)
    Replies: 4
    Last Post: 10-08-2013, 01:49 PM
  4. Penetration of weld and weld build up?
    By CGCINC in forum General Welding Questions
    Replies: 4
    Last Post: 07-03-2012, 07:06 AM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •