    I did my due diligence and saw no other posting on this. So here goes.......


    I recently ran out of tig rods and have around 10 lbs of gas welding rods. So I had a little project out of steel that needed some filler rod so I did a little test.

    Here is what I found. Do not use gas welding rods for tig. You will get porous welds with lots of pits and a very weak weld. I did a little research on this and found that tig rods have higher concentration of silicon and other de-oxidizers that are more suited for tig welding.

    I also tried the old standby for gas welding...the coat hanger. I suggest not using coat hangers any more even for gas welding. For tig, coat hangers should never be used as the metal they are made out of are probably your old Toyota with lots of crap in them. I tried one and I was amazed how bad the weld was. Like bird poop blobs everywhere.

    I then, just for the fun of it, decided to try mig wire. Specifically ER70S .30 wire. I tried a single strand and found controlling the flimsy wire was tough. So I took the wire, doubled it over and twisted it together with a cordless drill in effect doubling its diameter and making it fairly stiff. That seemed to work. The welding with that was smoother with no porosity at all.

    So in a pinch, if you really need to tig weld something say on a Saturday, are out of rods, the LWS is closed and have some mig wire laying around, it may be the answer.
    Powertig 250EX
    Powerplasma 50
    Hobart Handler 210 with spoolgun
    Cobra 2000 / Henrob O/A torch
    Drill press / metal brake / 36 ton air hydraulic press
    Franzinated modified Craftsman 33 compressor
    Lots of other metal working tools

  2. Default

    Thats interesting, thanks for the report.
    I have hear of using solid MIG wire for TIG before. I seem to recall that those were favorable reports also.
    Occasionally I weld some really small pieces, and the er70s2 1/16" rebar that I have is just too large. I've been meaning to try some of the solid MIG wire i have floating around.

  3. #3

    Default

    Mig wire works fine for Tig. I use it when I need small diameter stainless filler. I have never noticed any difference. The AWS designation on what I have is identical to Tig filler.

    What rods do you specifically use for gas welding? In the past, I just used tig rods for gas welding.
    Everlast 200DX
    Everlast PT185
    Shoptask 3-in-1 (not currently in my garage, but I own it...)

    Any day on a motorcycle like this that ends just needing parts and labor is a good day.
    4.82, 158.67mph 1/8th mile 7.350, 200.35mph 1/4 mile

  4. #4

    Default

    Quote Originally Posted by sportbike View Post
    Mig wire works fine for Tig. I use it when I need small diameter stainless filler. I have never noticed any difference. The AWS designation on what I have is identical to Tig filler.

    What rods do you specifically use for gas welding? In the past, I just used tig rods for gas welding.
    I use both 1/8 and 1/16 RG45 welding rods for mild steel. I'm using the Cobra 2000 (aka Henrob / Dillon torch). Those RG45 rods sure do not work well when tigging.

    I kind of figured out the problem with the welds as I used a rod on a test piece of metal and then an autogenous weld on the same test. The autogenous weld was beautiful but the weld that had RG45 rod added was really cratered and porous.

    I am of the opinion that tig welding is a very precise method of welding and that rules need to be followed. I will no longer even try to tig weld using gas rods. I am also of the opinion that gas welding is more forgiving and you can bend the rules and use tig rods.
    Powertig 250EX
    Powerplasma 50
    Hobart Handler 210 with spoolgun
    Cobra 2000 / Henrob O/A torch
    Drill press / metal brake / 36 ton air hydraulic press
    Franzinated modified Craftsman 33 compressor
    Lots of other metal working tools

  5. #5

    Default

    As well, in a pinch you can also use your aluminum MIG wire with the TIG.
    Mike R.
    Email: admineverlast@everlastwelders.com
    www.everlastgenerators.com
    www.everlastwelders.com
    877-755-9353 x203
    M-F 12 - 7PM PST
    FYI: PP50, PP80, IMIG-200, IMIG-250P, 210EXT and 255EXT.

  6. #6
    Join Date
    Sep 2011
    Location
    Home, Pa (Yes, that's the name of the town.)
    Posts
    121

    Default

    For welding sheet metal or other thin steel solid MIG wire works really well. Like the OP said though it is very hard to control being so thin. The mild steel TIG rods that I have are ER70S2 where as the solid MIG wire I got is ER70S6, I think that designates a higher silicon content, but it does work on thin steel very well if you can hold on to the thin wire. And just like using the ER70S6 MIG wire for thin steel, aluminum MIG wire works great on thin aluminum as well.
    Brad George
    George's Welding & Repair
    Amateur at TIG, MIG, and General Fabrication.
    Current Equipment
    AIRCO Heliwelder IV 300Amp Model - Total Awesomeness!
    Hobart Handler 120v MIG

  7. #7

    Default

    Quote Originally Posted by everlastsupport View Post
    As well, in a pinch you can also use your aluminum MIG wire with the TIG.
    or even better, when welding aluminum if you have any scraps or cutoffs of the actual base metal your welding, that is the best filler. sometimes it can be a pain working the scrap into something you can feed into the puddle, but putting base material back is the best. if you know, u have ran out of rod.
    Journeyman welder
    250EX
    Power plasma 60
    horizontal band saw
    Miller digital elite 'wicked' lid

  8. #8

    Default

    Done that with steel. The same steel, you can not get any better than that. I had a trailer bed (expanded metal) and I use the X piece to finish it off, I was to lazy to walk over and get more filler rod.
    Mike R.
    Email: admineverlast@everlastwelders.com
    www.everlastgenerators.com
    www.everlastwelders.com
    877-755-9353 x203
    M-F 12 - 7PM PST
    FYI: PP50, PP80, IMIG-200, IMIG-250P, 210EXT and 255EXT.

  9. #9

    Default

    Quote Originally Posted by jerky View Post
    or even better, when welding aluminum if you have any scraps or cutoffs of the actual base metal your welding, that is the best filler. sometimes it can be a pain working the scrap into something you can feed into the puddle, but putting base material back is the best. if you know, u have ran out of rod.
    For some alloys (including 6000 series) this is NOT recommend as it can lead to hot crasking issues. Welding of 6061 for example is usually done with 4043 for thinner materials, or 5356 filler for higher strength on thicker sections.

    It may not be an issue for decorative items or items where stress is not a concern, however filler metals as recommended by the Aluminum Association or similar should be used for anything that is load bearing.

    Also not a good idea for 4130 steel that will not be heat trreated after welding.
    Last edited by sportbike; 09-30-2011 at 05:28 PM.
    Everlast 200DX
    Everlast PT185
    Shoptask 3-in-1 (not currently in my garage, but I own it...)

    Any day on a motorcycle like this that ends just needing parts and labor is a good day.
    4.82, 158.67mph 1/8th mile 7.350, 200.35mph 1/4 mile

  10. #10
    Join Date
    Feb 2011
    Location
    Fridley, Minnesota
    Posts
    376

    Default

    I'm gonna go with sportbike on this one. The only time I have ever seen tig rod alloy matching the original base metal is the A356 rod that I paid $33.00/lb for to weld up an aluminum casting. I'm wondering if you could post pictures of your variable speed feeder with the hand-held end. I can see where if I could make something like that up, I'd end up using it more often than not.
    "It's not magic it's experimental, kind of like washing your hands after pooping used to be." -House

    Everlast PowerTig 250EX-arrived 1-26-2012
    Everlast PowerCool W300-arrived 1-26-2012
    Everlast PowerTig 185 Micro-arrived 1-26-2012
    Everlast PowerPlasma 70-arrived 1-26-2012
    ESAB MigMaster 250-borrowed
    HyperTherm 151 AKA "The Light Sabre"
    Linde UCC-305-964 lb. of old time water cooled TIG love-SOLD-Bad MOJO
    Purox OXY/ACETYLENE

  11. #11
    Join Date
    Mar 2011
    Location
    The Boonies of Texas
    Posts
    420

    Default

    Quote Originally Posted by hooda View Post
    I'm gonna go with sportbike on this one. The only time I have ever seen tig rod alloy matching the original base metal is the A356 rod that I paid $33.00/lb for to weld up an aluminum casting. I'm wondering if you could post pictures of your variable speed feeder with the hand-held end. I can see where if I could make something like that up, I'd end up using it more often than not.
    Harbor Freight has a cheap wire feeder that is readily adaptable to Tig. They call it a Mig Welder though .

    Thurmond
    Miller Bobcat 3 Phase,
    Miller Suitcase X-Treme 12VS wire feeder for the Bobcat with M-25 300A .045" gun / Bernard 400A 5/64" wire mig gun .
    26 series gas cooled TIG torch, setup for quick connect to Bobcat.
    17 series gas cooled Tig Torch for Low Amp Solar Tig (Direct Solar Panel Powered Tig welding)
    Hobart Handler 187 Mig / Fluxcore
    EVERLAST PowerUltra 205P
    EVERLAST PowerTig 250 EXT 2013 Model

  12. #12
    Join Date
    Feb 2011
    Location
    Fridley, Minnesota
    Posts
    376

    Default

    Quote Originally Posted by Tritium View Post
    Harbor Freight has a cheap wire feeder that is readily adaptable to Tig. They call it a Mig Welder though .

    Thurmond
    THAT is truly funny! Funnier yet is that it's true! But seriously a brilliant idea, if it will work with aluminum. I will put the idea high on my "to-do" list after I procure a new TIG welder. (was forced to sell the old linde). Without having to look it up, what's the going rate on HF's cheapest unit?
    "It's not magic it's experimental, kind of like washing your hands after pooping used to be." -House

    Everlast PowerTig 250EX-arrived 1-26-2012
    Everlast PowerCool W300-arrived 1-26-2012
    Everlast PowerTig 185 Micro-arrived 1-26-2012
    Everlast PowerPlasma 70-arrived 1-26-2012
    ESAB MigMaster 250-borrowed
    HyperTherm 151 AKA "The Light Sabre"
    Linde UCC-305-964 lb. of old time water cooled TIG love-SOLD-Bad MOJO
    Purox OXY/ACETYLENE

  13. #13

    Default

    For those whom want to use Mig wire maybe a tig pen would help.
    https://weldingsupply.securesites.co...UNDEF:X:TP1550
    I don't have one but for small filler rod it help.

    have fun
    Tom

    Everlast PM256
    Millermatic 180
    Hypertherm PowerMax 65 with machine torch
    Longevity Force Cut 80I
    DIY CNC table for plasma/routing
    13" metal lathe
    Small Mill
    ect, ect.

  14. #14

    Default

    We have a cold wire feeder in the shop at work that is used typical for GTAW machine track welding. We use it for Titanium test welds as well as some other welds. Pretty much required for automated, non autogeneous tig welding.

    I have also seen a small handheld end with a variable speed feeder for use when tig welding by hand, using spooled wire.
    Last edited by sportbike; 09-16-2011 at 02:42 PM.
    Everlast 200DX
    Everlast PT185
    Shoptask 3-in-1 (not currently in my garage, but I own it...)

    Any day on a motorcycle like this that ends just needing parts and labor is a good day.
    4.82, 158.67mph 1/8th mile 7.350, 200.35mph 1/4 mile

  15. #15

    Default

    I have only heard of good reports using MIG wire. Maybe rather than getting thin rods I will have to go get a spool of MIG wire and keep on hand for just this. I should have thought about that when I was tring to get some 309L locally and ended up with something to thick and had a tough time welding with it.
    Jason
    Everlast 255EXT - Perfection
    Everlast PowerPro 256 - UPS Demolished
    Everlast MTS200s
    12 Ton Shop Press
    DeWalt Hand Tools/ChopSaw

Similar Threads

  1. Rods to have on hand... which ones?
    By Trip59 in forum Stick Welding (SMAW)
    Replies: 29
    Last Post: 10-13-2012, 02:44 PM
  2. Free welding rods... help?
    By CGCINC in forum Stick Welding (SMAW)
    Replies: 17
    Last Post: 06-05-2012, 04:08 PM
  3. Small welding rods
    By Jules The Great in forum Stick Welding (SMAW)
    Replies: 9
    Last Post: 04-23-2012, 12:01 PM
  4. buy dinse conectors and welding rods
    By bobwills in forum General Welding Questions
    Replies: 8
    Last Post: 12-13-2011, 12:52 AM
  5. favorite brand of welding rods.
    By welderdude in forum General Welder Questions
    Replies: 13
    Last Post: 04-27-2011, 12:58 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •