    I welded some aluminum mounting studs onto some waterjet cut aluminum plate. Did two of these.
    Click image for larger version. 

Name:	IMG_0032_small.JPG 
Views:	704 
Size:	58.4 KB 
ID:	3187

    The waterjet-cut plate was 1/4" thick 6061-T6. Shown prior to welding the studs on:
    Click image for larger version. 

Name:	IMG_0021_small.JPG 
Views:	731 
Size:	107.9 KB 
ID:	3186

    The studs were 1/4-20 size, 5000 series aluminum; a good selection for high as-welded strength. The studs had a shoulder that I basically melted into the thick plate material autogenously (no filler rod added.) A shouldered weld-on stud, before and after welding:
    Click image for larger version. 

Name:	IMG_0031_small.JPG 
Views:	2255 
Size:	71.9 KB 
ID:	3185

    Settings: for maximum penetration, I went with an Ar/He mix (2.5 cfh He, 12.5 cfh Ar), and I used the torch switch to trigger a very brief, "all or nothing" 200 amps, along with the minimum cleaning (20% EP) AC Balance setting on my Super200P. I used a 1/16" tungsten with truncated point (sharp with flat.)

    I performed the welding in two passes:

    #1 - stuck the sharpened tungsten down very far in the fillet between the stud shoulder and flat plate - almost touching. Although often the puddle would melt onto the tungsten, it would ensure the two materials would successfully flow together (making a weak tack weld of sorts.)

    #2 - after cleaning off the aluminum contamination from the tip of the tungsten, I made a second pass around the welded area, holding the tungsten a bit further back this time, so the puddle did not touch it. I flashed the arc for a bit longer, making the puddle melt wider and most importantly, deeper, for increased penetration and added strength.

    Click image for larger version. 

Name:	IMG_0030_small.JPG 
Views:	849 
Size:	73.9 KB 
ID:	3184

    It's a pretty small, delicate part to weld onto a comparatively thick plate, but I would say this technique did the trick.

    Oh almost forgot, I used a welder's finger (Aka "third hand") to quickly hold the studs in position for the initial tack welds, and also for grounding. They are really useful for holding small aluminum pieces like these for tack welding.
    '13 Everlast 255EXT
    '07 Everlast Super200P

  2. #2
    Join Date
    Dec 2009
    Location
    Greater Seattle, WA
    Posts
    813

    Default

    I did some more of these, on thinner (1/8" thick) material, and the same size studs. It worked OK, using the same machine settings and technique, and just using pure argon instead of Ar/He mix instead, and perhaps holding the arc a bit longer on the second pass to get it to "melt in" better. I was a bit concerned about over penetrating into the 1/8" material with the Helium mix (and He is pricey, so not worth using unless its really needed.)

    Although the puddle didn't penetrate all the way through or anything, the 1/8" plate did deform ever so slightly; "rippling" the outline of the stud interface on the back side (which is the side that will actually show when these plates are "mounted".) It rippled from the relatively thinner material not being rigid enough to withstand the cooling-related contraction forces. It does show I got some decent penetration though, I think. Weld should be strong.
    '13 Everlast 255EXT
    '07 Everlast Super200P

  3. #3

    Default

    Looks easy until a person trys it, welding them plumb takes some doing. Nice work

  4. #4

    Default

    Is that your water jet?
    Lincoln Eagle Engine Drive
    Everlast MTS 250
    Everlast Power Tig 225lx
    HTP Mig 2400
    Everlast Power Plasma 60C --> Just need to finish my CNC Plasma Table!
    Miller Spectrum 375 Extreme Plasma cutter
    Victor cutting torch
    HF 20 Ton Shop Press
    HF 4x6 Band Saw
    HF Air Compressor
    Northern Tool Drill Press


    www.murphywelding.com

  5. #5
    Join Date
    Dec 2009
    Location
    Greater Seattle, WA
    Posts
    813

    Default

    Thanks, Geezer.

    SeanMurphy - the customer supplied them already waterjet cut.
    '13 Everlast 255EXT
    '07 Everlast Super200P

  6. #6

    Default

    Could you weld these without filler rod, just using the lip on the stud as filler?(I know it's not a big lip) Maybe set to pulse and go slow around the stud?

    Just wondering for my personal knowledge.....
    PowerTig 250EX
    Power I-MIG 200
    Power Plasma 50
    It's what you learn, After you know it all, that counts!

  7. #7
    Join Date
    Dec 2009
    Location
    Greater Seattle, WA
    Posts
    813

    Default

    That's how I did it. (No filler rod.) I did another batch of these since I posted this.
    '13 Everlast 255EXT
    '07 Everlast Super200P

  8. #8

    Default

    Quote Originally Posted by jakeru View Post
    That's how I did it. (No filler rod.) I did another batch of these since I posted this.

    Ohhh, Cool..... Good to know!
    PowerTig 250EX
    Power I-MIG 200
    Power Plasma 50
    It's what you learn, After you know it all, that counts!

Similar Threads

  1. Using Helium for Aluminum Wheel Repair (jakeru's #19)
    By jakeru in forum Welding Repairs
    Replies: 16
    Last Post: 02-18-2012, 04:29 AM
  2. Aluminum Cartop Boat Transom Gussets (jakeru's #16)
    By jakeru in forum Welding Repairs
    Replies: 4
    Last Post: 01-20-2012, 02:23 PM
  3. Replies: 4
    Last Post: 10-09-2011, 10:39 PM
  4. Replies: 2
    Last Post: 08-03-2011, 03:50 PM
  5. Aluminum Boat Fishing Rod Mounting Plates (jakeru's #8)
    By jakeru in forum Other Custom Fabrications
    Replies: 6
    Last Post: 06-28-2011, 09:10 AM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •