    It's Sunday morning, and I am looking forward to building a Stainless steel kickstand for the Egli project. I have thought about the design for a couple of days and I'm ready to go. Almost.

    I forgot that the last time I used the Wellsaw the blade broke. I don't have a spare at the moment and the Industrial suppliers are all closed.
    It was still cutting like new when it broke. It got jammed in some 1 3/4" solid stock I was cutting to build a 75 HP. pto shaft for my tractor mower.

    I was ready to write the day off to lawn mowing and weed eating rather than metal work then thought I should try tig welding the blade back together. Some metal cutting bandsaws have blade welders built right into the machine , don't they?

    It's back on there and cutting nicely. It will be interesting to see if the weld holds up.
    The filler rod I used was some 1/16" 309L stainless. I can't tell you what is happening Metallurgically when using 309L on a bimetal blade, but it seemed like it might just work, given past experience.

    Glen
    Attached Thumbnails Attached Thumbnails Click image for larger version. 

Name:	002.jpg 
Views:	723 
Size:	124.3 KB 
ID:	2644   Click image for larger version. 

Name:	004.jpg 
Views:	724 
Size:	136.0 KB 
ID:	2645   Click image for larger version. 

Name:	001.jpg 
Views:	690 
Size:	146.1 KB 
ID:	2646   Click image for larger version. 

Name:	003.jpg 
Views:	705 
Size:	147.2 KB 
ID:	2647   Click image for larger version. 

Name:	005.jpg 
Views:	678 
Size:	137.4 KB 
ID:	2648  

    Last edited by worntorn; 07-04-2011 at 12:22 AM.
    Everlast PP256
    Everlast Imig 200
    Everlast Power Ultra 205
    P&H 400 amp A.C.
    Miller 230 amp with Onan power

  2. #2
    Join Date
    Dec 2009
    Location
    Greater Seattle, WA
    Posts
    813

    Default

    A bandsaw blade I TIG welded a couple months ago is still holding like a champ!
    http://www.everlastgenerators.com/fo...Bandsaw-Blades
    '13 Everlast 255EXT
    '07 Everlast Super200P

  3. #3

    Default

    Hi Jake

    Looks like you came up with a similar method for holding things with your 2nd method.

    This blade is a bimetal blade so I figured it might be hard to weld.
    It wasn't really, it was just a case of starting the arc low (10 amps) then pushing the pedal a bit until things start to flow.

    There is one small trick for welding small profile material like this. This was shown to me by a welding instructor. If you light up on the filler rod rather than the item to be welded, then you have a better chance to gauge the amount of heat needed without destroying the item. The filler rod forms a small molten ball first, then you add amperage carefully until the filler and the two blade pieces flow together. As soon as this happens start moving. In about 1 second you are done!

    Glen
    Everlast PP256
    Everlast Imig 200
    Everlast Power Ultra 205
    P&H 400 amp A.C.
    Miller 230 amp with Onan power

  4. #4
    Join Date
    Dec 2009
    Location
    Greater Seattle, WA
    Posts
    813

    Default

    Yep, jigging the blade for welding with "nothing but air" on the backside of the weld, and using relatively low current to allow heat to soak and build into the blade material and getting the whole weld area glowing red hot (and also allow it to cool slowly) is what worked well to weld my high carbon blade material while keeping the welded area soft and annealed.

    I've used the trick of a short, quick burst of heat over the end of a filler rod, to deposit a controlled, small amount of the rod right where you want it to go, with minimal heat input to the part. (It's a great way to patch a small hole in very thin material.) I'll have to try the "slow heat build up over filler rod" idea sometime. I would imagine that would allow the tip of the tungsten to come up to operating temperature, and stabilize the arc for low-current welding. Actually I would like to try that on aluminum sometime.
    '13 Everlast 255EXT
    '07 Everlast Super200P

Similar Threads

  1. Bandsaw blade questions?
    By CGCINC in forum General Welding Questions
    Replies: 9
    Last Post: 11-05-2012, 01:44 PM
  2. Project # 11 from Worntorn: Ossa Fenders
    By worntorn in forum Personal Projects (no welder required)
    Replies: 1
    Last Post: 07-27-2011, 02:13 AM
  3. Project # 8 from Worntorn- another driveway gate setup
    By worntorn in forum Other Custom Fabrications
    Replies: 3
    Last Post: 06-23-2011, 08:49 PM
  4. Replies: 0
    Last Post: 06-20-2011, 06:54 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •