    Got this rod called A356. Supposed to be for casting repair. think it acts like regular 4043. but it costs $27.00/lb.!!! anyone know anything about it?
    "It's not magic it's experimental, kind of like washing your hands after pooping used to be." -House

    Everlast PowerTig 250EX-arrived 1-26-2012
    Everlast PowerCool W300-arrived 1-26-2012
    Everlast PowerTig 185 Micro-arrived 1-26-2012
    Everlast PowerPlasma 70-arrived 1-26-2012
    ESAB MigMaster 250-borrowed
    HyperTherm 151 AKA "The Light Sabre"
    Linde UCC-305-964 lb. of old time water cooled TIG love-SOLD-Bad MOJO
    Purox OXY/ACETYLENE

  2. #2

    Default

    A356 is a grade of cast aluminum.
    Everlast lx225
    Hobart Handler 210 with spool gun
    Hobart Stickmate LX
    Thermal Arc 400GMS
    40 amp Northern Tools plasma torch
    130 chicago electric tig welder
    90 amp chicago electric flux mig
    10"-22" Grizzly lathe
    15"-5.5" Grizzly vertical end mill

    In need of nice TIG machine. drooling over PowerTig 250ex

  3. #3
    Join Date
    Dec 2009
    Location
    Greater Seattle, WA
    Posts
    813

    Default

    As I understand it, A356 is a common alloy used for many sand-cast aluminum parts. You can identify sand-cast parts often by their "rough" texture. (Like automotive cylinder heads, intake manifolds, etc.) If your aiming to repair auto and motorcycle castings, you'll come across plenty of it!

    At 7% Silicon content, it has a just below eutectic mixture in it. It also has some Magnesium in it (.38%), the combination of these two ingredients make it heat treatable. And also, be aware when welding it, can make it weak in the heat affected zone. Some strength may regain over time (from "natural aging".)

    According to the Alcotec aluminum filler rod selection chart, A356 filler rod is useful for welding A356 and other similar cast parent alloys. In comparison to 4043, it has a slight edge on tensile strength earning it an "A" rating for that application, versus 4043's "B" rating on same application. This may be helpful for a sand cast aluminum application where you need all the as-welded strength you can muster and is worth the extra replacement cost.

    Another alloy to be aware of as an option for welding sand cast aluminum, is 4047. It is often sold as a brazing rod; and its basically a eutectic mix of Aluminum+12% Silicon. Its supposed to work well for welding cast aluminum, even though its not officially recognized on the Alcotec chart as a welding alloy for that application or any other aluminum welding application (why, I don't know.) I haven't tried it, but have heard good things. It melts at a low temperature and when it melts, its completely melted (not much of a "slushy" range, between the solidus and liquidus temperatures.)
    '13 Everlast 255EXT
    '07 Everlast Super200P

Similar Threads

  1. why does my arc get funky when filler rod gets near
    By JohnT in forum TIG Welding (GTAW/GTAW-P)
    Replies: 5
    Last Post: 04-05-2018, 04:02 PM
  2. New to welding. Which filler rod?
    By Xman4u in forum General Welding Questions
    Replies: 2
    Last Post: 01-16-2015, 11:43 AM
  3. Where to buy magnesium tig filler rod???
    By Brian Ski in forum General Welding Questions
    Replies: 12
    Last Post: 04-17-2014, 06:41 PM
  4. Late Christmas Gift PowerTig 210EXT Need some answers Please.......
    By JohnM019R in forum TIG Welding (GTAW/GTAW-P)
    Replies: 10
    Last Post: 12-31-2013, 03:59 PM
  5. TIG Filler
    By bigjoeinkg in forum TIG Welding (GTAW/GTAW-P)
    Replies: 13
    Last Post: 07-18-2011, 09:50 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •