This is my first of many attempt at welding 6" diameter 1/4" thick steel pipe in the 2g position. I beveled both edges, but didnt have the best fitup. I ran the first pass with a 1/8 inch 6011 at 80 amps dcep where the gap was big and 95 amps dcep where the gap was small. I ran the next two passes with a 3/32 7018 at 90 amps dcep. Due to the crappy fitup, I didnt always get a nice keyhole. I plan on doing some more practicing later on.



 
					
					 
							