    what rods are best for welding cast iron? i know that when it gets hot then cools it cracks then splits and pops. i've used a OA torch to preheat then welded with special rods. nothing seems to work so far
    Aaron

  2. #2

    Default

    Use a nickel rod with low heat, keep your weld length to 1/2 to 1 inch long and use a ball peen hamer to relive the stress, or use a cast rod again keeping the weld length short to prevent stress cracks. Use light bead build up and clean and chip before you apply a second bead on the buildup

  3. #3

    Default

    Aaron, take a look at www.weldingtipsandtricks.com Mr. Jody Collier discusses welding on cast at some length. You might get ideas from him as to how to proceed. You can also email him directly if you need specific questions answered.

    Z
    PowerTig 225LX
    PowerCool W300
    PowerPlasma 60S
    Miller 140 MIG

  4. #4
    Join Date
    Dec 2009
    Location
    Greater Seattle, WA
    Posts
    813

    Default

    There are quite a few different techniques I've read about for welding cast... bronze filler rod vs nickel vs. stainless steel vs. cast iron filler rod, pre-heat, post-heat, peening weld with hammer.

    I'm planning on tackling welding to a gray cast iron exhaust manifold here pretty soon.

    I'm planning on attempting it with "Nickel 55" (a 55% nickel) rod and some pre/post heat with a "weed burner" oxy-propane torch. The 55% nickel rods (with balance material nearly all iron) are designed specifically for joining cast iron to other cast iron or to steel, and are readily available at my local welding supplies in 1/8" flux covered stick welding electrode format.

    I haven't decided yet if I'm going to:
    A. stick weld it
    B. TIG weld it using the stick electrode (including flux) as a filler rod
    C. TIG weld it using the "bare" stick electrode (flux manually removed) as a filler rod.

    I sourced some bare "nickel 55" TIG filler rods via mail order, but found they were quite a bit more expensive, and with twice as high of a minimum ordering quantity than the stick electrodes of the same alloy composition.
    '13 Everlast 255EXT
    '07 Everlast Super200P

  5. #5

    Default

    Cast iron welding by preheating the whole part in an oven to about 300 degrees F, doing the welding (re-heating if multi passes or a long weld is needed), then putting the whole thing in a vermiculite filled container. Vermiculite is available for use in garden soil and is almost like small styrofoam packing peanuts. The vermiculite insulates the part and basically allows it to cool slowly.

    Not sure I need to mention this, but DO NOT USE STYROFOAM PACKING PEANUTS :-)

    John
    Everlast 200DX
    Everlast PT185
    Shoptask 3-in-1 (not currently in my garage, but I own it...)

    Any day on a motorcycle like this that ends just needing parts and labor is a good day.
    4.82, 158.67mph 1/8th mile 7.350, 200.35mph 1/4 mile

Similar Threads

  1. Cast Iron Car block tig welded
    By Kempy in forum Welding Repairs
    Replies: 18
    Last Post: 06-20-2023, 10:22 AM
  2. question on welding cast iron
    By revkev6 in forum TIG Welding (GTAW/GTAW-P)
    Replies: 4
    Last Post: 02-26-2017, 02:18 PM
  3. Repairing a small cast iron gib key
    By build in forum General Welder Questions
    Replies: 8
    Last Post: 12-13-2012, 02:23 AM
  4. Cast Iron
    By Estarial in forum General Welding Questions
    Replies: 13
    Last Post: 07-15-2011, 05:36 PM
  5. bandsaw repair, cast iron
    By starvingartist in forum Welding Repairs
    Replies: 1
    Last Post: 06-24-2011, 02:29 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •